Cleaning materials: PC regrind material (for high temperature use), PP (for low temperature use), PMMA regrind material, PE or cleaning agent.
Cleaning timing:
Before changing colors or switching to different types of raw materials.
When the previous color powder residue in the pipe is not cleaned properly.
When there are many carbides (black spots) in the molded products. When cleaning the previous color powder residue in the pipe:
Increase the temperature of the color powder injection by 10-20°C because the remaining color powder needs to be hotter than the plastic temperature to blend in. Stop cooling the feed inlet with cooling water.
Increase the temperature control point at the cooling part of the feed inlet by 10°C-20°C. Color powder is sticky and tends to get stuck in the screw groove.
Use PMMA regrind material, set the temperature of the front section to 260 degrees, and perform 5-8 purge/filling cleaning cycles.
Or use PC regrind material, set the temperature to 290-300 degrees, and perform 5-8 purge/filling cleaning cycles.
After cleaning the material pipe, remove the nozzle, use a blowtorch to clean the nozzle, and then harden it by soaking it in water.
When cleaning PA (PA6), HDPE or PP cleaning materials can be used, and the temperature should be set at 240-250 degrees.
When cleaning PA66, PC regrind material can be used, and the temperature should be set at 300-320 degrees.
Points to note for cleaning material pipes: